TPC-ET at Shore D 64 with a 214 °C melting point, 50 MPa stress at break and MFI 20, for injection molding and extrusion.
Sipolprene 61220 is a thermoplastic copolyester elastomer (TPC-ET) at Shore D 64, with a 214 °C melting point and a melt flow of 20 g/10 min at 230 °C, 2.16 kg. Sipol designed it as a medium-modulus ether ester elastomer with a rheology suited to injection molding and extrusion.
Stress at break is 50 MPa and elongation at break 400 percent, with notched Izod no break at 23 °C. The 214 °C melting point sits 2 °C above Sipolprene 60212 and 3 °C above 63210.
Its crystallization temperature is 145 °C, 69 degrees below the melt and well below the 179 °C of Sipolprene 60212 and 178 °C of 65215 on either side of it in hardness.
Sipol's data sheet for 61220 is short. It gives no flexural modulus, glass transition, Vicat, cold impact, abrasion or compression set values, and it carries no food contact statement. If your part depends on any of those, ask before you specify the grade.
Sipol has no separate data sheet for a 61220 version. Black, UV-stabilized and heat-stabilized dry blends are available on request.
It is also written as TPC-ET, thermoplastic copolyester elastomer, TPEE, TEEE, COPE, copolyester elastomer, thermoplastic polyester elastomer, and ether ester elastomer.
| Property | Typical value |
|---|---|
| Melting temperature | 214 °C (ISO 11357-3) |
| Crystallization temperature | 145 °C (ISO 11357-3) |
| Melt flow index (MFI) | 20 g/10 min at 230 °C, 2.16 kg (ISO 1133) |
| Melt volume rate (MVR) | 15 cm³/10 min at 230 °C, 2.16 kg (ISO 1133) |
| Shore D hardness | 64 instantaneous, 61 after 15 s (ISO 868) |
| Stress at break | 50 MPa (ISO 527) |
| Elongation at break | 400 % (ISO 527) |
| Notched Izod impact at 23 °C | No break (ISO 180) |
| Density | 1.23 g/cm³ (ISO 1183) |
| Water absorption | 0.2 % after 24 h immersion at 23 °C (Sipol method MI 08) |
| Form | Granules |
| Versions | Black, UV-stabilized and heat-stabilized dry blends on request |
Typical values from the manufacturer's technical data sheet. They describe the product, they are not a specification. We will send the current TDS and the batch documentation your qualification needs.
Tell us the part or the process, the property you are targeting, and the volume you expect. We will confirm the grade, send the documentation, and get a sample of the candidate grade to you.
Sipol's profile runs 200 °C at the rear zone up to 225 °C at the nozzle, with the mold at 30 to 40 °C.
The extrusion profile climbs from 195 to 210 °C at the feed to 210 to 225 °C at the head and die.
Sipol supplies black, UV-stabilized and heat-stabilized dry blends on request.
Dry before processing. Sipol recommends 2 to 3 hours at 90 °C in a dehumidifying dryer and gives a processing moisture content of 0.15 percent.
For injection molding, Sipol suggests the rear zone at 200 °C, the center zone at 210 °C, the front zone at 220 °C and the nozzle at 225 °C, with the mold at 30 to 40 °C.
For extrusion, the suggested profile is feed zone 195 to 210 °C, compression zone 210 to 220 °C, metering zone 210 to 225 °C and head or die 210 to 225 °C.
Package sizes: 25 kg bags with an aluminum film moisture barrier, 500 kg cardboard octabins with an inner PE liner, and 500 kg or 1000 kg big bags..
Storage: Stable for 12 months unopened in the original packaging, kept in a cool, dry place and protected from light. Material held at around 5 to 10 °C or below should sit at 15 to 20 °C for at least 24 hours before use.
Read the safety data sheet before handling.
Sipolprene 61220 melts at 214 °C. For injection molding Sipol suggests 200 °C at the rear zone, 210 °C center, 220 °C front and 225 °C at the nozzle, with the mold at 30 to 40 °C. For extrusion the profile runs 195 to 210 °C at the feed, 210 to 220 °C in compression, and 210 to 225 °C through metering and the die. Dry first for 2 to 3 hours at 90 °C in a dehumidifying dryer.
Sipol's sheet for Sipolprene 61220 gives melting and crystallization temperatures, melt flow, Shore D 64, 50 MPa stress at break, 400 percent elongation, notched Izod at 23 °C, density and water absorption. It gives no flexural modulus, glass transition, Vicat, -40 °C impact, abrasion or compression set. Tell us which of those your part depends on and we will ask Sipol for the data before you commit.
Sipol's data sheet for Sipolprene 61220 carries no food contact statement, so we make no food contact claim for it. In the same hardness band, Sipolprene 63210 at Shore D 62 and 65215 at Shore D 65 are both stated by Sipol to be in compliance with American FDA and European EU 10/2011 food contact regulations in their natural versions.
Sipolprene 61220 is Shore D 64 against 62 for 63210, melts at 214 °C against 211 °C, and has a higher stress at break, 50 MPa against 48 MPa. Sipolprene 63210 flows more at MFI 23 against 20 g/10 min, has a full published property set including 320 MPa flexural modulus, an HV extrusion version, and an FDA and EU 10/2011 food contact statement.
Yes. We send the Technical Data Sheet (TDS) and Safety Data Sheet (SDS) on request, in the manufacturer's current revision. Use Request TDS or SDS above and tell us what your qualification review needs.
Shore D 62 with a full property set and an HV extrusion version.
Shore D 60 high-modulus grade at 460 MPa, with a food contact statement.
Shore D 65 at 470 MPa, with a 215 °C melt.
The Sipolprene range by hardness and melting point, and where copolyester elastomer does not fit.
What the TPC-ET name means and how copolyester elastomer differs from TPU.
Matching an existing specification by Shore D hardness, melt viscosity and version suffix.