Sipolprene 60212

High-modulus TPC-ET at Shore D 60 with a 212 °C melting point, 460 MPa flexural modulus and 235 N/mm tear strength. Natural grade FDA and EU 10/2011.

Home › Products › Sipol › Sipolprene 60212

Sipolprene 60212 is a thermoplastic copolyester elastomer (TPC-ET) at Shore D 60, with a 212 °C melting point and a melt flow of 21 g/10 min at 230 °C, 2.16 kg. Sipol designed it as a high-modulus ether ester elastomer with a rheology suited to injection molding and extrusion.

The natural grade carries Sipol's standard stabilization package and, per Sipol's data sheet, is in compliance with American FDA and European EU 10/2011 food contact regulations.

Flexural modulus is 460 MPa, well above the 280 MPa of Sipolprene 58210 two Shore points below it, and tear strength is 235 N/mm (ASTM D 1004). Stress at break is 45 MPa and elongation at break 450 percent.

Notched Izod is no break at 23 °C and 20 J/m at -40 °C, so the grade suits parts that see room-temperature impact. A part that takes impact in deep cold should be tested at its service temperature. Abrasion loss is 45 mm³ (ISO 4649).

Crystallization temperature is 179 °C. Sipol has no separate data sheet for a 60212 version; black, UV-stabilized and heat-stabilized dry blends are available on request.

It is also written as TPC-ET, thermoplastic copolyester elastomer, TPEE, TEEE, COPE, copolyester elastomer, thermoplastic polyester elastomer, and ether ester elastomer.

Typical properties

PropertyTypical value
Melting temperature212 °C (ISO 11357-3)
Crystallization temperature179 °C (ISO 11357-3)
Melt flow index (MFI)21 g/10 min at 230 °C, 2.16 kg (ISO 1133)
Melt volume rate (MVR)17 cm³/10 min at 230 °C, 2.16 kg (ISO 1133)
Shore D hardness60 instantaneous, 58 after 15 s (ISO 868)
Stress at break45 MPa (ISO 527)
Elongation at break450 % (ISO 527)
Flexural modulus460 MPa (ISO 178)
Tear strength235 N/mm (ASTM D 1004)
Notched Izod impact at 23 °CNo break (ISO 180)
Notched Izod impact at -40 °C20 J/m (ISO 180)
Abrasion loss45 mm³ at 5 N vertical load (ISO 4649)
Density1.22 g/cm³ (ISO 1183)
Water absorption0.2 % after 24 h immersion at 23 °C (Sipol method MI 08)
ColorNatural
FormGranules
VersionsBlack, UV-stabilized and heat-stabilized dry blends on request

Typical values from the manufacturer's technical data sheet. They describe the product, they are not a specification. We will send the current TDS and the batch documentation your qualification needs.

Need this in your system?

Tell us the part or the process, the property you are targeting, and the volume you expect. We will confirm the grade, send the documentation, and get a sample of the candidate grade to you.

Applications

Injection molded parts

Sipol's profile runs 200 °C at the rear zone up to 225 °C at the nozzle, with the mold at 30 to 40 °C.

Extruded parts

The extrusion profile climbs from 195 to 210 °C at the feed to 210 to 225 °C at the head and die.

Food-contact parts

The natural grade is stated in compliance with FDA and EU 10/2011 food contact regulations.

Black, UV and heat-stabilized parts

Sipol supplies black, UV-stabilized and heat-stabilized dry blends on request.

Handling and dispersion

Dry before processing. Sipol recommends 2 to 3 hours at 90 °C in a dehumidifying dryer and gives a processing moisture content of 0.15 percent.

For injection molding, Sipol suggests the rear zone at 200 °C, the center zone at 210 °C, the front zone at 220 °C and the nozzle at 225 °C, with the mold at 30 to 40 °C.

For extrusion, the suggested profile is feed zone 195 to 210 °C, compression zone 210 to 220 °C, metering zone 210 to 225 °C and head or die 210 to 225 °C.

Packaging, storage, and regulatory status

Package sizes: 25 kg bags with an aluminum film moisture barrier, 500 kg cardboard octabins with an inner PE liner, and 500 kg or 1000 kg big bags..

Storage: Stable for 12 months unopened in the original packaging, kept in a cool, dry place and protected from light. Material held at around 5 to 10 °C or below should sit at 15 to 20 °C for at least 24 hours before use.

Sipol states the natural grade is in compliance with American FDA and European EU 10/2011 food contact regulations. Read the safety data sheet before handling.

Frequently asked questions

What processing temperatures does Sipolprene 60212 need?

Sipolprene 60212 melts at 212 °C. For injection molding Sipol suggests 200 °C at the rear zone, 210 °C center, 220 °C front and 225 °C at the nozzle, with the mold at 30 to 40 °C. For extrusion the profile runs 195 to 210 °C at the feed, 210 to 220 °C in compression, and 210 to 225 °C through metering and the die. Dry first for 2 to 3 hours at 90 °C in a dehumidifying dryer.

How stiff is Sipolprene 60212?

Sipolprene 60212 has a flexural modulus of 460 MPa at Shore D 60, and Sipol classes it as high modulus. That is 140 MPa above Sipolprene 63210 at Shore D 62 and close to the 470 MPa of Sipolprene 65215 at Shore D 65. Tear strength is 235 N/mm by ASTM D 1004, and elongation at break is 450 percent.

How does Sipolprene 60212 handle cold impact?

Sipolprene 60212 shows no break in notched Izod at 23 °C and 20 J/m at -40 °C (ISO 180). For a part that takes impact well below freezing, Sipolprene 58210 reads 80 J/m and 63210 reads 82 J/m at -40 °C, at lower flexural modulus. Test the finished part at its lowest service temperature before you commit.

Is Sipolprene 60212 food-contact compliant?

Sipol's data sheet states that natural Sipolprene 60212, with its standard stabilization package, is in compliance with American FDA and European EU 10/2011 food contact regulations. Black, UV-stabilized or heat-stabilized dry blends are not covered by that statement on the sheet, so specify the natural grade for a food-contact part and ask for the food contact declaration with the TDS and SDS.

Can I get the TDS and SDS for Sipolprene 60212?

Yes. We send the Technical Data Sheet (TDS), Safety Data Sheet (SDS), and Food contact declaration (FDA, EU 10/2011) on request, in the manufacturer's current revision. Use Request TDS or SDS above and tell us what your qualification review needs.

Related products

Sipolprene 63210

Shore D 62 at 320 MPa, with better cold impact and an HV extrusion version.

Sipolprene 65215

Shore D 65 at 470 MPa, the next high-modulus grade up.

Sipolprene 61220

Shore D 64 with a 214 °C melt and 50 MPa stress at break.

Where this grade fits

TPC-ET copolyester elastomers

The Sipolprene range by hardness and melting point, and where copolyester elastomer does not fit.

What is TPC-ET

What the TPC-ET name means and how copolyester elastomer differs from TPU.

Matching a TPC-ET specification

Matching an existing specification by Shore D hardness, melt viscosity and version suffix.

Evaluating Sipolprene 60212?

Tell us the system you are formulating and the property you need to hit. We will confirm the grade, send the data sheet, and ship a sample.