Shore D 38 ether ester TPC-ET melting at 170 °C, with melt flow of 10 g/10 min at 190 °C. Natural grade meets EU 10/2011 food contact regulation.
Sipolprene 40171 is an ether ester thermoplastic elastomer (TPC-ET) at a nominal Shore D 38, with a melting temperature of 170 °C. Sipol rates its melt behavior as suitable for injection molding and extrusion.
Flexural modulus is 50 MPa, stress at break 22 MPa and elongation at break 380 percent. Notched Izod shows no break at 23 °C or -40 °C, with a glass transition of -35 °C, and the Vicat A softening point is 103 °C.
Compression set is 22 percent at 23 °C and 62 percent at 70 °C. Abrasion loss is 51 mm³ at 5 N.
Water absorption is 3.2 percent after 24 hours of immersion at 23 °C, against 0.7 percent for Sipolprene 35150 and 35180, and the data sheet calls for 3 to 4 hours of drying where those two call for 2 to 3. Melt flow is 10 g/10 min measured at 190 °C and 2.16 kg.
The natural grade comes with a standard stabilization package, and Sipol states it is in compliance with European EU 10/2011 food contact regulation. Sipolprene 40171 B is the black dry blend on its own data sheet with the same property table. UV-stabilized and heat-stabilized dry blends are available on request.
It is also written as TPC-ET, thermoplastic copolyester elastomer, TPEE, TEEE, COPE, copolyester elastomer, thermoplastic polyester elastomer, and ether ester elastomer.
| Property | Typical value |
|---|---|
| Melting temperature | 170 °C (ISO 11357-3) |
| Crystallization temperature | 101 °C (ISO 11357-3) |
| Glass transition temperature | -35 °C (ISO 11357-2) |
| Vicat softening, A/50 | 103 °C (ISO 306) |
| Melt flow index (MFI) | 10 g/10 min at 190 °C, 2.16 kg (ISO 1133) |
| Melt volume rate (MVR) | 8 cm³/10 min at 190 °C, 2.16 kg (ISO 1133) |
| Shore D hardness | 38 instantaneous, 35 after 15 s (ISO 868) |
| Stress at break | 22 MPa (ISO 527) |
| Elongation at break | 380 percent (ISO 527) |
| Flexural modulus | 50 MPa (ISO 178) |
| Notched Izod impact, 23 °C | No break (ISO 180) |
| Notched Izod impact, -40 °C | No break (ISO 180) |
| Abrasion resistance | 51 mm³ at 5 N vertical load (ISO 4649) |
| Compression set, 23 °C | 22 percent (ISO 815:1991) |
| Compression set, 70 °C | 62 percent (ISO 815:1991) |
| Density | 1.18 g/cm³ (ISO 1183) |
| Water absorption | 3.2 percent, 24 h immersion at 23 °C (Sipol method MI 08) |
| Color | Natural; black in the B dry blend |
| Versions | 40171 natural, 40171 B black dry blend; UV and heat stabilized dry blends on request |
Typical values from the manufacturer's technical data sheet. They describe the product, they are not a specification. We will send the current TDS and the batch documentation your qualification needs.
Tell us the part or the process, the property you are targeting, and the volume you expect. We will confirm the grade, send the documentation, and get a sample of the candidate grade to you.
Shore D 38 with a 50 MPa flexural modulus, molded at 175 to 195 °C barrel temperatures.
Extrusion profile of 160 to 170 °C at the feed and 170 to 185 °C at the die.
The natural grade is stated in compliance with EU 10/2011 food contact regulation.
Dry before processing at 90 °C for 3 to 4 hours in a dehumidifying dryer, to a processing moisture content of 0.15 percent. With 3.2 percent water absorption after 24 hours of immersion, keep to the longer drying time on this data sheet.
Suggested injection molding profile for a 170 °C melting grade: rear zone 150 to 165 °C, center zone 175 °C, front zone 185 °C and nozzle 195 °C, with the mold at 20 to 30 °C.
Suggested extrusion profile: feeding zone 160 to 170 °C, compression zone 170 to 180 °C, metering zone 170 to 185 °C and head or die 170 to 185 °C.
Package sizes: 25 kg bags with an aluminum film moisture barrier, 500 kg cardboard octabins with an inner PE liner, and 500 kg and 1000 kg big bags..
Storage: Stable for 12 months unopened in the original packaging, kept cool and dry and protected from light. Material held at around 5 to 10 °C or below should sit at 15 to 20 °C for at least 24 hours before use.
Sipol states the natural grade, with its standard stabilization package, is in compliance with European EU 10/2011 food contact regulation. The data sheet carries no FDA statement, and the 40171 B dry blend sheet carries no food contact statement. Read the safety data sheet before handling.
Sipolprene 40171 calls for 3 to 4 hours at 90 °C in a dehumidifying dryer, to a processing moisture content of 0.15 percent. That is longer than the 2 to 3 hours on the Sipolprene 35150 and 35180 data sheets, and it fits the grade's water absorption of 3.2 percent after 24 hours of immersion at 23 °C.
Sipolprene 40171 melts at 170 °C. Sipol suggests an injection barrel profile of 150 to 165 °C at the rear zone, 175 °C center, 185 °C front and 195 °C at the nozzle, with the mold at 20 to 30 °C. The extrusion profile runs 160 to 170 °C at the feed and 170 to 185 °C at the die. Melt flow is 10 g/10 min at 190 °C and 2.16 kg.
Sipol states that the natural Sipolprene 40171, with its standard stabilization package, is in compliance with European EU 10/2011 food contact regulation. The data sheet does not mention FDA, so we do not describe the grade as FDA compliant. The 40171 B black dry blend carries no food contact statement on its own sheet.
Sipolprene 40171 melts at 170 °C against 150 °C for Sipolprene 35150, at almost the same hardness, Shore D 38 against 37, and the same 50 MPa flexural modulus. Both carry an EU 10/2011 statement and both measure melt flow at 190 °C. 35150 is the grade developed for PVC blending; 40171 stretches less, 380 percent against 570 percent, and absorbs more water.
Yes. We send the Technical Data Sheet (TDS), Safety Data Sheet (SDS), and Food contact declaration (EU 10/2011) on request, in the manufacturer's current revision. Use Request TDS or SDS above and tell us what your qualification review needs.
Shore D 37 melting at 150 °C, developed for plasticizer-free PVC blends, also EU 10/2011.
Shore D 35 melting at 177 °C, with FDA and EU 10/2011 statements and an HV version.
Shore D 45 melting at 209 °C, with the same 3 to 4 hour drying time.
The Sipolprene range from soft to hard, and where copolyester elastomer fits against TPU.