Sipolprene 35150

Shore D 37 block ether ester TPC-ET with a 150 °C melting point, developed for blending with PVC into plasticizer-free soft compounds. EU 10/2011 food contact.

Home › Products › Sipol › Sipolprene 35150

Sipolprene 35150 is a block ether ester thermoplastic elastomer (TPC-ET) at a nominal Shore D 37, with a low modulus and a melting temperature of 150 °C. Sipol developed it specifically with a low melting point, which makes it suitable for blending with PVC to make soft compounds free of plasticizer.

The low melting point carries through to processing. Sipol's suggested injection profile runs 130 to 145 °C at the rear zone and 175 °C at the nozzle, and the extrusion profile holds 155 to 170 °C at the die, with melt flow measured at 190 °C.

On its own it molds and extrudes as a Shore D 37 elastomer with a 50 MPa flexural modulus, 28 MPa stress at break and 570 percent elongation. Notched Izod shows no break at 23 °C or -40 °C, and the glass transition is -55 °C.

Vicat A softening is 105 °C. Compression set is 24 percent at 23 °C and 76 percent at 70 °C, so check the warm figure against any part that has to hold a seal.

The natural grade comes with a standard stabilization package, and Sipol states it is in compliance with European EU 10/2011 food contact regulations. Sipolprene 35150 B is the black dry blend, and Sipolprene 35150 P has its own data sheet with the same property table and the same PVC-blending and EU 10/2011 statements. UV-stabilized and heat-stabilized dry blends are available on request.

It is also written as TPC-ET, thermoplastic copolyester elastomer, TPEE, TEEE, COPE, copolyester elastomer, thermoplastic polyester elastomer, and ether ester elastomer.

Typical properties

PropertyTypical value
Melting temperature150 °C (ISO 11357-3)
Crystallization temperature74 °C (ISO 11357-3)
Glass transition temperature-55 °C (ISO 11357-2)
Vicat softening, A/50105 °C (ISO 306)
Melt flow index (MFI)9 g/10 min at 190 °C, 2.16 kg (ISO 1133)
Melt volume rate (MVR)8 cm³/10 min at 190 °C, 2.16 kg (ISO 1133)
Shore D hardness37 instantaneous, 33 after 15 s (ISO 868)
Stress at break28 MPa (ISO 527)
Elongation at break570 percent (ISO 527)
Flexural modulus50 MPa (ISO 178)
Notched Izod impact, 23 °CNo break (ISO 180)
Notched Izod impact, -40 °CNo break (ISO 180)
Abrasion resistance33 mm³ at 5 N vertical load (ISO 4649)
Compression set, 23 °C24 percent (ISO 815:1991)
Compression set, 70 °C76 percent (ISO 815:1991)
Density1.15 g/cm³ (ISO 1183)
Water absorption0.7 percent, 24 h immersion at 23 °C (Sipol method MI 08)
ColorNatural; black in the B dry blend
Versions35150 natural, 35150 B black dry blend, 35150 P; UV and heat stabilized dry blends on request

Typical values from the manufacturer's technical data sheet. They describe the product, they are not a specification. We will send the current TDS and the batch documentation your qualification needs.

Need this in your system?

Tell us the part or the process, the property you are targeting, and the volume you expect. We will confirm the grade, send the documentation, and get a sample of the candidate grade to you.

Applications

Plasticizer-free soft PVC compounds

Sipol developed 35150 with a low melting point for blending with PVC into soft compounds without plasticizer.

PVC compounding

Melting at 150 °C, with melt flow of 9 g/10 min measured at 190 °C.

Food contact compounds and parts

The natural grade and 35150 P are stated in compliance with EU 10/2011 food contact regulations.

Injection molded and extruded parts

Shore D 37 with a 50 MPa flexural modulus, processed at 175 °C or below.

Handling and dispersion

Dry before processing at 90 °C for 2 to 3 hours in a dehumidifying dryer, to a processing moisture content of 0.15 percent.

Suggested injection molding profile for a 150 °C melting grade: rear zone 130 to 145 °C, center zone 155 °C, front zone 165 °C and nozzle 175 °C, with the mold at 20 to 30 °C.

Suggested extrusion profile: feeding zone 140 to 150 °C, compression zone 150 to 160 °C, metering zone 155 to 170 °C and head or die 155 to 170 °C.

Packaging, storage, and regulatory status

Package sizes: 25 kg bags with an aluminum film moisture barrier, 500 kg cardboard octabins with an inner PE liner, and 500 kg and 1000 kg big bags..

Storage: Stable for 12 months unopened in the original packaging, kept cool and dry and protected from light. Material held at around 5 to 10 °C or below should sit at 15 to 20 °C for at least 24 hours before use.

Sipol states the natural grade, with its standard stabilization package, and 35150 P are in compliance with European EU 10/2011 food contact regulations. The data sheet carries no FDA statement, and the 35150 B black dry blend sheet carries no food contact statement. Read the safety data sheet before handling.

Frequently asked questions

What is Sipolprene 35150 designed for?

Sipolprene 35150 was developed specifically with a low melting point, 150 °C, which makes it suitable for blending with PVC to make soft compounds free of plasticizer. It is a Shore D 37 block ether ester TPC-ET, and Sipol rates it for injection molding and extrusion as well. Blend ratios and blend properties are not on the data sheet; they are worked out on the customer's compound.

What temperatures does Sipolprene 35150 need?

Sipolprene 35150 melts at 150 °C. Sipol suggests an injection barrel profile of 130 to 145 °C at the rear zone, 155 °C center, 165 °C front and 175 °C at the nozzle, with the mold at 20 to 30 °C. The extrusion profile runs 140 to 150 °C at the feed and 155 to 170 °C at the die. Dry it at 90 °C for 2 to 3 hours first, to 0.15 percent moisture.

Is Sipolprene 35150 food-contact compliant?

Sipol states that the natural Sipolprene 35150, with its standard stabilization package, is in compliance with European EU 10/2011 food contact regulations, and the 35150 P data sheet carries the same statement. Neither sheet mentions FDA, so we do not describe the grade as FDA compliant. The 35150 B black dry blend carries no food contact statement.

What separates Sipolprene 35150 from Sipolprene 25150?

Both data sheets state the PVC-blending purpose and a 150 °C melting point. Sipolprene 35150 is harder at Shore D 37 against Shore D 24, stiffer at 50 MPa flexural modulus against 17 MPa, and carries an EU 10/2011 food contact statement and a black dry blend that Sipolprene 25150 does not list. 25150 flows faster, 19 g/10 min at 200 °C.

Can I get the TDS and SDS for Sipolprene 35150?

Yes. We send the Technical Data Sheet (TDS), Safety Data Sheet (SDS), and Food contact declaration (EU 10/2011) on request, in the manufacturer's current revision. Use Request TDS or SDS above and tell us what your qualification review needs.

Related products

Sipolprene 25150

The softer PVC-blending grade, Shore D 24 at the same 150 °C melting point.

Sipolprene 40171

Shore D 38 melting at 170 °C, also EU 10/2011, with melt flow measured at 190 °C.

Sipolprene 35180

Shore D 35 melting at 177 °C, with FDA and EU 10/2011 statements and an HV version.

Where this grade fits

TPC-ET copolyester elastomers

The Sipolprene range from soft to hard, and where copolyester elastomer fits against TPU.

What is TPC-ET

What the TPC-ET name means and how the family differs from TPU.

Matching a TPC-ET specification

How to match a copolyester elastomer specification by hardness, melt flow and version.

Evaluating Sipolprene 35150?

Tell us the system you are formulating and the property you need to hit. We will confirm the grade, send the data sheet, and ship a sample.